Products |
|
|
|
|
|
|
Properties of PIM Stainless Steels and Low Alloy Steels:
Material(Condition) |
Minimum Values |
Typical Values |
Tensile Properties |
|
|
ρ
(g/cm3) |
Hardness |
σ b
(MPa) |
σ 0.2
(MPa) |
δ
(%) |
σ b
(MPa) |
σ 0.2
(MPa) |
δ
(%) |
PIM-316L as-sintered |
448 |
138 |
40.0 |
517 |
172 |
50 |
7.6 |
HRB67 |
PIM-17-4PH as-sintered |
793 |
648 |
4.0 |
896 |
731 |
6 |
7.5 |
HRC27 |
PIM-17-4PH solution treated and aged |
1069 |
965 |
4.0 |
1186 |
1089 |
6 |
7.5 |
HRC33 |
PIM-4600 as-sintered |
255 |
110 |
20.0 |
290 |
124 |
40 |
7.6 |
HRB45 |
PIM-4650 as-sintered |
379 |
172 |
11.0 |
441 |
207 |
15 |
7.5 |
HRB62 |
PIM-4650 quenched & tempered |
1482 |
1310 |
1.0 |
1655 |
1482 |
2 |
7.5 |
HRC48 |
PIM-2700 as-sintered |
379 |
207 |
20.0 |
414 |
255 |
26 |
7.6 |
HRB69 |
|
|